This paper considers the use of the yeast Saccharomyces cerevisiae as a biosorbent for the recovery of gold from Mahd El-Dahhab gold mine in Kingdom of Saudi Arabia. Gold is a noble metal which was seldom used in electroplating, hydrogenation catalyst, etc. Heterogeneous composition of samples and low concentration offer renewed interest in the selective extraction of gold using various extractants. In the present work, Saccharomyces cerevisiae , is used to study the preconcentration of gold, which in the original sample was 0.44 ppm, while after treatment with Saccharomyces cerevisiae it raises to 7 ppm with efficiency reaching about 1600%.
Gold, the noblest one of metals, has been used by man for more than 5000 years. Its extreme softness or malleability, and resistance to tarnish (oxidation), led to its earliest use in art and currency. Gold is the metal of choice for jewelers, and is often used in dentistry. Gold has been successfully used in many modern technological applications. It is used as the electrical contacts of computer chips. Minute quantities of gold (less than 3 micrograms) are vaporized to mirror lens surfaces [
Minor concentrations of gold occur in most natural substances. In seawater, for example, there is approximately 0.012 parts per billion (ppb) of gold and in fresh water it is slightly higher at 0.02 ppb. Its average concentration in the Earth’s crust or lithosphere is approximately 5 ppb, and in certain sedimentary rocks it may achieve concentrations of up to 2100 ppb or 2.1 parts per million (ppm).
Mahd El Dahab is an epithermal, low sulphidation, adularia type, polymetallic deposit. The total production has been estimated at over 100 tons of gold [
Systematic rock geochemistry over a 50 m × 50 m grid discovered new reserves [
Four successive alteration stages are observed: early alteration with quartz, sericite, pyrite; an intermediate stage with chlorite, sericite, microcline, sphalerite, pyrite; the gold bearing stage with quartz, chlorite, sphalerite, galena, pyrite, gold, tellurides, and accessory siderite-calcite-hematite and a final stage with quartz, calcite, and barite. Minor (apparently) gold indications are known from near Mahd Adh Dhahab, as Lahuf [
Extraction of gold from solutions is under active investigation by using a variety of physical, chemical, and biological processes. Recovery of ionic gold from dilute solutions usually involves either precipitation by zinc dust, carbon adsorption, solvent extraction, or ion exchange resins. All of these are of low selectivity and comparatively expensive [
Biorecovery of dissolved gold from solution presents fewer environmental risks than chemical methods, and is documented for microorganisms [
The ore contained 8.2% Fe, 0.78% Cu, 0.88% As, and 0.035% with pyrite, hematite, arsenopyrite, and chalcopyrite as the main metal-bearing minerals. Initial gold recovery by conventional cyanidation on a crushed ore sample was 54%; concentration by flotation improved recovery to 56%. Concentrated samples (17.0 g Au/ton) were leached in reactors at pH 1.8. In the presence of bacteria, all dissolved iron was presented as ferric ion; gold recovery by cyanidation increased from 13% for the initial concentrate to 97% after 10 days of bacterial leaching. To further increase gold recovery, flotation tailings were submitted to cyanidation [
Algal cells, alive or dead, rapidly accumulated Au3+ and begin to reduce it to Au0 and Au+ within 2 days [
Gold (Au3+) can be sequestered from acid solutions by dead biomass of a brown alga, Sargassum natans (Linnaeus), and deposited in its elemental form, Au0.
The cell wall of Sargassum was the major locale for gold deposition, with carbonyl groups (C=O) playing a major role in binding, and N-containing groups have lesser role. Like activated carbon, the biomass of Sargassum natans is extremely porous, reportedly more than most biomaterials, and accounts, in part for its ability to accumulate gold [
The bioreduction of Au+3 to Au0 using biomass of the brown alga Fucus vesiculosus was investigated. The recovery and reduction process took place in two stages with an optimum pH range of 4 - 9 with a maximum uptake obtained at pH 7 [
The effects of ionic gold on Saccharomyces cerevisiae, extension of preincubation time of yeast cells in gold- containing medium resulted in a decreasing proton efflux rate and colloidal phase formation in the cell suspensions. The time between gold addition and the beginning of colloidal phase formation depended on the gold concentration used. Both Ca and Mg enhanced the inhibitory effect of gold on the yeast cells with Ca showing a stronger inhibitory effect than Mg [
- Mahd El Dahab sampling:
Sample in this work was kindly obtained from Mahd El Dahab mine, Kingdom of Saudi Arabia.
- The organisms used in this work.
Saccharomyces cerevisiae used in this work was provided by EL-Hwamdiyah Company of Yeast and Sugar, Giza, Egypt. It is cultivated in (glucose-peptone-yeast extracts broth) medium which composition is
Yeast extracts 3 g L
Peptone 3 g L
Glucose 10 g L
Agar 15 g L
Dist. water 1000 ml.
The obtained glucose-peptone-yeast-extracts agar media was melted and poured into Petri dishes and then left to solidify, by using a sterile inoculation needle a loop full of one of colonies was taken and streaked on the surface of the solidified agar plates, followed by incubation for 72 hours at 30˚C. Sub culture was prepared by addition of pure Saccharomyces colonies on slants of glucose-peptone yeast agar.
- Preparation of liquid media:
An amount of 100 ml of glucose-peptone yeast extract previously prepared medium were added to 100 gm of Mahd Ad Dahab gold sample and let for incubation for 10 day at 30˚C. All flasks were sealed with removable cotton. Temperature was kept in the incubator at 28˚C - 30˚C during the experiment.
After separation the media, the result of Mahd Ad Dahab gold sample was dried and weighted then subjected to different analysis to identify the elements and groups which were affected by Saccharomyces cerevisiae.
- Sample analysis
The collected sample was identified through four collaborative techniques.
Fire assay has been in use for thousands of years and still stands the test of time as the standard method to value noble metals. A lot of attention are given to “micron gold” or “colloidal gold”. A cold hard fact of this type of gold requires a lot of material to make even one ounce. Generally, much more ore than an independent operator is equipped to move. No machine, recovery process, or chemical method will produce any gold if there are not enough values to collect it from the ore.
The ore must, in all case, be reduced to a state of fine powder so as to pass through at least a 60 mesh sieve. The metallic residues they must be carefully collected and cupelled separately with lead.
Pyritic ores: they are treated either by preliminary roasting at a low temperature until sweep and then treated just as the ores with basic gangues, or they may be fused at once with a heavy charge of red lead, and little or no charcoal.
A suitable charge would be:
Ore 50 gram
Red lead 60 gram
Borax 20 gram
Sodium carbonate 40 gram
A little sand may be added if silica is not already presented, and care must be taken to thoroughly saturate the charge with metallic iron. The precautions already referred to as to fritting of the charge, and the treatment of the button must be carefully absorbed. The sample was treated with fire assay before and after treatment with Saccharomyces cerevisiae
Environmental scanning electron microscope (ESEM), Philips XL 30 was applied for brief qualitative investigation of minerals in each sample for quick semi quantitative of the obtained products under the usual conditions at low vacuum. And voltage from 5 - 30 KV, the back scatter electron detector (BSE), and occasionally gas scatter electron detector (GSE) were used for photomicrographs. The attached unit of energy dispersive X-ray (EDX) was used to obtain the semi quantitative chemical analysis.
The samples are subjected to Infrared spectroscopy in order to determine the function groups of the samples. The used instrument is Naxux 670 FTIR, Company name (Nicollet) USA. The range of spectrum is usually performed from 4000 to 400 Cm−1, with resolution 4 Cm−1.
XRD was used to identify the unknown minerals using instrument Philips PW3710/31 diffract meter with automatic sample changer PW1775, (21 positions) scintillation counter, Cu-target tube and Ni filter at 40 KV and MA. This instrument is connected to a computer system using X-40 diffraction program and ASTM cards for mineral identification in NMA.
The Saccharomyces sp. is one of the best studied and commercially exploited of all microorganisms [
The roles of the ions in yeast cells are twofold:
1) Enzymatic functioning as part of the catalytic centre of an enzymes, as activators of enzyme activity and as physiological regulators. Zinc, cobalt, manganese and copper are common in catalytic centres; magnesium acts as an enzyme activator and potassium commonly functions as a metal co-enzyme;
2) A structural function. Potassium and magnesium have a role in neutralizing electrostatic interactions between cellular anionic units of polyphosphates, DNA, RNA and proteins [
The presence of cations in yeast is significant with respect to its exploitation as a metal biosorbent. Yeast cells require metals for normal metabolic processes and readily accumulate a range of metals. The second point relates to the delicate intracellular ionic balance, with imbalances being reflected as alterations in metabolic processes and growth characteristics. Exposure of yeast from malt fermentation to high levels of metals in a bioremediation system would possibly lead to cell death and further metal removal would be by metabolism independent mechanisms.
The cell wall and plasma membrane are the most important components of the yeast cell in metal removal from aqueous solutions. The cell wall maintains structure and rigidity and is permeable to solutes smaller than 600 Dalton. It serves as the initial contact point and provides the negative functional groups for cation binding. The yeast cell wall consists of an intermesh of polysaccharide microfibrils in a matrix of various polysaccharides, proteins and lipids. The major constituent (~60%) of the cell wall is the polysaccharide mixture of glucans, phosphomannans and chitin [
Chemical and enzymatic isolation of the cell wall components of Saccharomyces cerevisiae indicates metal binding to each of the cell wall components. The isolated components accumulate greater quantities of cations than intact cells, with the outer mannan-protein layer being identified as more important for metal binding than the inner chitin layer [
In contrast to bacteria with a single plasma membrane, Saccharomyces cerevisiae cells contain a number of specialized membranes. Most important to metal transport are the outer membrane separating the cell components from the external medium and the vacuolar membrane which compartmentalizes different metabolically important compounds [
Transport of solutes through the membrane is mediated by primary and secondary transport proteins. Primary transport is the active process in which chemical energy is converted to electrochemical energy [
Fire assay is used for the determination of gold before and after treatment with Saccharomyces cerevisiae the original gold content in the sample is 0.44 ppm and reach a higher value 7 ppm as shown in
Au Before (ppm) | Au After (ppm) |
---|---|
0.44 | 7 |
volcanic rocks with gold and sulphides, while
The cell wall of Saccharomyces cerevisiae was the major locale for gold accumulation. Treatment with Saccharomyces cerevisiae on Mahd Ad Dahab gold sample in infra red instrument notified the presence of functional group OH, Ch aliphatic, Co acidic and C-O-C, after action with Saccharomyces cerevisiae we notice the appearance of two function groups (CO imide & SO2), with the disappearance of C=C after microbial action as appeared in
Gold is a noble metal, the term “noble metal” means that the metal will not oxidize or react with most acids. Mahd adh Dhabab is one of the largest gold mine in the Arabian world, the estimated reserve are around 1.2 MT of gold with an average grade of 24 g/t. The sample provided from the mine is taken at one of the richest part of the mine, it is noticed that the abundance of chalcopyrite in the original sample decreases after treatment in big amount. Saccharomyces cerevisiae action on the sample leads to recovery of gold from 0.44 ppm to 7 ppm with efficiency reaching about 1600% from the original sample.
Nora Shenouda Gad,Mahmoud H. Shalaby, (2015) Microbial Recovery of Gold from Mahd El-Dahab Mine Kingdom of Saudi Arabia. Open Access Library Journal,02,1-9. doi: 10.4236/oalib.1101440